- ISO 9001 - 2015 Certified
- PED 2014/68/EC
- NACE MR0175/ISO 15156-2
- NORSOK M-650
- DFAR
- MERKBLATT AD 2000 W2/W7/W10
Duplex (ferritic-austenitic) stainless steel bolting grade, furnished solution annealed
UNS S32205 (Type 2205) is one of the 14 duplex (ferritic-austenitic) stainless steels in ASTM A1082/A1082M (2016), the specification for high strength bolting for special purpose applications such as pressure vessels. Table 1 sets chromium 22.0-23.0 %, nickel 4.5-6.5 %, molybdenum 3.0-3.5 % and N 0.14-0.20. Table 4 requires tensile strength 95 ksi [655 MPa] min, yield strength 65 ksi [450 MPa] min, elongation 25 % min and hardness 30 HRC or 290 HB max. Duplex grades are furnished in the solution-annealed condition (clause 7.2.1): 1900 °F [1040 °C] ±25 °F [15 °C], quenched in water (Table 4). The marking grade symbol is 32205 (Table 5).
| Grades | UNS Designation | Type | C | Mn | P | S | Si | Cr | Ni | Mo | N | Other ElementsB |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| ASTM A1082/A1082M Duplex (Ferritic-Austenitic) Grades | S32205 | 2205 | 0.030 | 2.00 | 0.030 | 0.020 | 1.00 | 22.0-23.0 | 4.5-6.5 | 3.0-3.5 | 0.14-0.20 | . . . |
|
||||||||||||
| UNS Designation | Solution Temperature, °F [°C] (B, C) | Tensile Strength, min, ksi [MPa] | Yield Strength, 0.2% offset, min, ksi [MPa] | Elongation in 2" [50 mm] or 4D, min, % | Rockwell HRC, max | Brinell max (D) |
|---|---|---|---|---|---|---|
| S32205 | 1900 [1040] | 95 [655] | 65 [450] | 25 | 30 | 290 |
|
||||||
| UNS Designation | Type | Grade Symbol |
|---|---|---|
| S32205 | 2205 | TB 32205 |
S32205 is a duplex (ferritic-austenitic) stainless steel listed in ASTM A1082/A1082M Table 1 as Type 2205, with chromium 22.0-23.0 %, nickel 4.5-6.5 %, molybdenum 3.0-3.5 % and N 0.14-0.20. A1082 covers bars, bolts and nuts in this grade for special purpose applications such as pressure vessels; ASTM A962/A962M general requirements also apply.
Table 4 requires tensile strength 95 ksi [655 MPa] min, yield strength 65 ksi [450 MPa] min, elongation 25 % min and hardness 30 HRC or 290 HB max.
ISO 15156-3 Table A.24 accepts wrought duplex stainless steel for any equipment when it is solution-annealed and liquid-quenched or rapidly cooled, has 35 % to 65 % ferrite and has had no ageing heat treatment. With 30 ≤ PREN ≤ 40 and Mo ≥ 1.5 % the limit is 232 °C (450 °F) and 10 kPa (1.5 psi) H2S partial pressure; with 40 < PREN ≤ 45 it is 232 °C (450 °F) and 20 kPa (3 psi). PREN is calculated from the heat's actual analysis, and ISO 15156-3 sets no HRC maximum for wrought duplex.
Duplex grades are furnished in the solution-annealed condition (clause 7.2.1): 1900 °F [1040 °C] ±25 °F [15 °C], quenched in water (Table 4). The marking grade symbol is 32205 (Table 5).